| 耐气候影响性能良好,可回收材料,耐疲劳性能,耐化学性良好,耐臭氧性能,尺寸稳定性良好,抗紫外线性能良好 片材挤出成型,挤出,挤出吹塑成型,注吹成型,吹塑成型,注射成型,热成型,真空成型,型材挤出成型,多次注射成型,共挤出成型 | 黑色 |
| 汽车领域的应用,室外应用 | |
| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | |
| 比重 | ASTMD792 | 0.968 | g/cm3 | |
| 密度 | ISO1183 | 0.970 | g/cm3 | |
| 室外适用性 | UL746C | f1 | ||
| DetergentResistance | UL2157 | f4 | ||
| DetergentResistance | UL749 | f3 | ||
| 弹性体 | TestMethod | NominalValue | Unit | |
| 拉伸应力-横向流量(100%应变,23°C) | ASTMD412 | 4.60 | MPa | |
| 拉伸应力-横向流量(100%应变,23°C) | ISO37 | 4.60 | MPa | |
| 抗张强度-横向流量(断裂,23°C) | ASTMD412 | 11.0 | MPa | |
| TensileStress-AcrossFlow(Break,23°C) | ISO37 | 11.0 | MPa | |
| 伸长率-横向流量(断裂,23°C) | ASTMD412 | 560 | % | |
| 伸长率-横向流量(断裂,23°C) | ISO37 | 560 | % | |
| 撕裂强度-横向流量2(23°C) | ASTMD624 | 35.0 | kN/m | |
| TearStrength-AcrossFlow3(23°C) | ISO34-1 | 35 | kN/m | |
| CompressionSet4 | 23°C,22hr | ASTMD395B | 25 | % |
| CompressionSet4 | 125°C,70hr | ASTMD395B | 52 | % |
| 压缩永久变形4 | 23°C,22hr | ISO815 | 25 | % |
| 压缩永久变形4 | 125°C,70hr | ISO815 | 52 | % |
| 肖氏硬度(邵氏A,15秒,23°C) | ISO868 | 85 | ||
| 脆化温度 | ASTMD746 | -59.0 | °C | |
| 脆化温度 | ISO812 | -59.0 | °C | |
| RTIElec | UL746 | 90.0 | °C | |
| RTIStr | 1.0mm | UL746 | 90.0 | °C |
| RTIStr | 1.5mm | UL746 | 90.0 | °C |
| RTIStr | 3.0mm | UL746 | 95.0 | °C |
| ChangeinTensileStrengthinAir(135°C,1008hr) | ASTMD573 | -3.0 | % | |
| ChangeinTensileStrengthinAir(135°C,1008hr) | ISO188 | -3.0 | % | |
| ChangeinUltimateElongationinAir(135°C,1008hr) | ASTMD573 | -10 | % | |
| ChangeinTensileStrainatBreakinAir(135°C,1008hr) | ISO188 | -10 | % | |
| ChangeinDurometerHardnessinAir(ShoreA,135°C,1008hr) | ASTMD573 | 7.0 | ||
| ChangeinShoreHardnessinAir(ShoreA,135°C,1008hr) | ISO188 | 7.0 | ||
| ChangeinTensileStrength(125°C,70hr,inIRM903Oil) | ASTMD471 | -33 | % | |
| ChangeinTensileStress(125°C,70hr,inIRM903Oil) | ISO1817 | -33 | % | |
| ChangeinUltimateElongation(125°C,70hr,inIRM903Oil) | ASTMD471 | -48 | % | |
| ChangeinTensileStrainatBreak(125°C,70hr,inIRM903Oil) | ISO1817 | -48 | % | |
| 体积变化(125°C,70hr,在IRM903油中) | ASTMD471 | 67 | % | |
| 体积变化(125°C,70hr,在IRM903油中) | ISO1817 | 67 | % | |
| ContinuousUpperTemperatureResistance(1008hr) | SAEJ2236 | 135 | °C | |
| DielectricStrength(23°C,2.00mm) | ASTMD149 | 28 | kV/mm | |
| DielectricConstant(23°C,1.96mm) | ASTMD150 | 2.60 | ||
| DielectricConstant(23°C,1.96mm) | IEC60250 | 2.60 | ||
| 相比耐漏电起痕指数(CTI) | UL746 | PLC0 | ||
| 高电弧燃烧指数(HAI) | UL746 | PLC0 | ||
| 高压电弧抗点燃指数(HVAR)(PLC) | UL746 | PLC6 | ||
| 高电压电弧起痕速率(HVTR) | UL746 | PLC1 | ||
| 热丝引燃(HWI) | 1.0mm | UL746 | PLC4 | |
| 热丝引燃(HWI) | 1.5mm | UL746 | PLC3 | |
| 热丝引燃(HWI) | 3.0mm | UL746 | PLC2 | |
| UL阻燃等级 | 1.0mm | UL94 | HB | |
| UL阻燃等级 | 1.5mm | UL94 | HB | |
| UL阻燃等级 | 3.0mm | UL94 | HB | |
TPV 121-80塑料供应商,长期销售美国埃克森美孚生产的TPV原料,以上是“TPV 121-80”塑胶料的物性表参数.近期代理商可转仓交易:德国科思创 PC/ABS FR3000 注塑
● TPV 意大利SO.F.TER. 6EK.A85
汽车部件,挤出
● TPV 土耳其Elastron Elastron V V101.A55.B
耐化学性良好,柔软,可粘结性,注射成型,挤出
● TPV 美国KMI Elastoprene 70A-1000
● TPV 埃克森美孚 8281-45MED 其它
● TPV 意大利Taroplas 1 A60 M1N
性能特点:可回收材料, 可加工性良好。